TIG WELDING CARBON STEEL 1/4 THICK CORNER JOINT PULSE ROOT

Free download TIG WELDING CARBON STEEL 1/4 THICK CORNER JOINT PULSE ROOT LAYWIRE TECHNIQUE video and edit with RedcoolMedia movie maker MovieStudio video editor online and AudioStudio audio editor onlin

This is the free video TIG WELDING CARBON STEEL 1/4 THICK CORNER JOINT PULSE ROOT LAYWIRE TECHNIQUE that can be downloaded, played and edit with our RedcoolMedia movie maker MovieStudio free video editor online and AudioStudio free audio editor online

VIDEO DESCRIPTION:

Play, download and edit the free video TIG WELDING CARBON STEEL 1/4 THICK CORNER JOINT PULSE ROOT LAYWIRE TECHNIQUE.

WELD PROCESS = TIG, GTAW, GAS TUNGSTEN ARC WELDING

METAL TYPE = carbon steel

THICKNESS = .250”
WELD TYPE = FILLET

JOINT TYPE = CORNER JOINT

POSITION = 2F

AMPERAGE = MACHINE AMPS SET TO 200 CONTROLLED WITH FOOT PEDAL

TUNGSTEN = 2% LANTHANATED, 3/32"

FILLER WIRE = 3/32” ER70S2

POLARITY = DCEN

GAS FLOW = 20 CFH argon

CUP SIZE = 8

PRE FLOW = .5 SEC

POST FLOW = 7 SEC

ADDITIONAL SETTINGS = PULSE SETTINGS 1PPS, 40% BACKGROUND, 50% ON TIME

TIPS: KEEP A TIGHT ARC

Aim for an arc length that is equal or less than the diameter of your tungsten electrode.

Torch angle can be forgiving provided your arc length is tight.

Keep the hot tip of the filler wire shielded by the argon envelope from the tig cup

Snip oxidized tip of filler metal before a restart